A saddle is fused onto the outside of a pipe that is already in the ground, often already live, and it can never be moved afterwards. The procedure is short but the preparation and the cooling time carry almost all of the result. This is the sequence we recommend, and the points where it goes wrong.
Why saddle fusion is not pipe fusion
A saddle is fused to the outside of a pipe that is already in the ground and already full. That changes four things about the weld.
| Pipe or fitting fusion | Saddle fusion | |
|---|---|---|
| Surfaces in contact | Two flat or cylindrical faces of the same geometry | A curved saddle body against a curved pipe outside |
| Heating | Heater plate, or a coil inside a socket | A coil moulded into the saddle body only |
| What holds it in position | The machine, or the pipe stiffness | A clamp: the saddle has to be held against the pipe through the whole cycle |
| What the pipe is doing | Empty, usually | Often live, and always unable to move |
Because the fit between two curved surfaces is never as good as the fit inside a socket, the clamp and the surface preparation carry more of the result than they do on a pipe joint. A saddle that is not clamped down during the cycle will give a joint that looks fused and leaks at the edge.
Before the weld
| Check | What to do | Why |
|---|---|---|
| Main is round and sound | Inspect the area the saddle will sit on; reject dents, deep scratches and ovality | The saddle cannot conform to a distorted pipe, and the gap becomes a leak path |
| Surface is clean | Wipe the full contact area, then scrape the oxide layer off | The fusion surface is the pipe outside, so it has to be prepared like one |
| Correct model and size | Confirm the saddle matches the main OD, and whether it is the old or the new model | The two models have different ranges and are not interchangeable |
| Clamp fits | Dry-fit the clamp and the saddle before the cycle | A clamp that has to be forced distorts the saddle before the coil heats it |
| Coil and terminals undamaged | Look at the coil ends; a broken terminal means the saddle is scrap | The circuit is the weld: there is no second chance once current is applied |
| Control box matched | The box has to be the one the saddle's barcode or data sheet is written for | A cycle from the wrong box is the wrong amount of energy |
The procedure, step by step
- Mark the position on the main: the centre of the outlet, and the orientation. A saddle fused in the wrong place cannot be moved.
- Prepare the surface over the whole contact area, not just under the outlet. Scrape, then wipe clean.
- Dry-fit and clamp. Seat the saddle, fit the clamp, and check that the outlet points where it should.
- Connect the coil to the control box and confirm the cycle: barcode scan, or the parameters from the saddle data sheet.
- Run the cycle without interruption. Do not adjust or re-seat the saddle while current is flowing.
- Let it cool fully before removing the clamp. On a live main this is the step people rush, and it is the step that decides the joint.
- Check the melt indicator where the saddle has one: it shows that the material reached fusion temperature.
- Tap the main through the outlet, with the tool that matches the outlet size, and withdraw the coupon.
- Check the coupon: a full disc of the main wall means the hole is complete and round. A partial coupon or a torn one means the tap was not clean.
Tapping the main
| Point | Correct | If it is wrong |
|---|---|---|
| Tool size | Matched to the outlet, not to the branch pipe | A step in the bore that catches pigs, scrapers and swabs |
| Tool condition | Sharp cutter, correct for PE | A torn coupon and a ragged hole edge |
| Advance rate | Steady, without forcing | Heat build-up and smearing at the hole edge |
| Coupon | Full disc, kept as evidence of a complete hole | No coupon means no proof the hole is through and clean |
| Sealing after withdrawal | Tool's own seal, then the outlet is capped or connected | An open outlet on a live main |
The outlet is then fused to the branch pipe, or capped if the branch is not being made yet. On a gas main the outlet is a record item: which saddle, which cycle, which coupon.
What a good joint looks like, and what a bad one looks like
| Sign | Meaning | Action |
|---|---|---|
| Melt indicator raised or clear | Fusion temperature was reached | Proceed |
| Even fillet of melt around the saddle edge | Material melted across the whole footprint | Proceed |
| No melt visible at one edge | Clamp lifted early, or the surface was not prepared there | Cut out and replace; do not tap |
| Saddle distorted or rocked | Clamp was forced, or released during the cycle | Replace |
| Burnt or discoloured material at the coil | Wrong cycle: too much energy | Replace, and check the control box settings |
| Gap visible under the saddle body | Pipe out of round, or wrong saddle model for the OD | Replace with the correct model, or move to a sound section of main |
Frequently asked questions
Can a saddle be fused to a live main?
Yes, that is what it is for. Electrofusion puts no heat source outside the saddle and nothing moves, so the main can stay in service. The clamp has to be held through the cycle and the cooling time, and the tap is made after the joint has cooled.
What is the cooling time for a saddle?
It is in the saddle data sheet and it depends on the size, so it is not a single number. The practical rule is that the clamp stays on until the joint is fully cool, not until it looks solid.
Can I re-fuse a saddle that failed?
No. A saddle is consumed by the joint. The failed one is cut off, and the replacement goes on a sound section of the main, which sometimes means moving the tapping point along the pipe.
Do I have to keep the tapping coupon?
On a gas network, yes: the coupon is the evidence that the hole is complete and the wall was cut cleanly, and it is part of the record. On water it is good practice and costs nothing.
What size tapping tool do I need?
One matched to the saddle outlet, not to the branch pipe. A dn63 outlet takes a dn63 tool even if the branch reduces further downstream.
- HDPE saddle sizes – clamp, bypass and end plug, with branch sizes and both models
- HDPE fittings for gas distribution – where saddles are used on live mains
- How HDPE pipes are joined – electrofusion on pipe and fitting
- HDPE fittings installation guide – preparation, testing and backfill
- HDPE fittings specifications – every family as a full table