Butt Fusion Welding Parameters For HDPE Pipe: Temperature, Pressure, Time And Bead Size
Nov 03, 2026
Leave a message
Four values decide whether an HDPE joint holds: plate temperature, the three pressures, the four time values, and the bead that forms while the first three are working. Get them right and the joint outlives the pipe. Get them roughly right and the joint passes a pressure test and fails a year later.
The values below are the ones we issue with our machines, plus the way crews adjust them when the site is not a laboratory. Method selection first: butt fusion or electrofusion.
Plate Temperature Depends On The Compound, Not On Habit
220 °C is not universal, and a crew that welds at 220 °C summer and winter is guessing. The plate temperature follows the compound grade, because melt behaviour differs between them. PE100 and PE80 do not fuse on the same schedule.
| Pipe grade | Plate temperature | Note |
|---|---|---|
| PE100 | 225 ± 10 °C | Standard condition, ambient 5-35 °C |
| PE80 | 210 ± 10 °C | Lower melt flow, lower plate setting |
| Ambient below 5 °C | +5 to +10 °C | Compensates heat loss in transfer |
| Above 38 °C, direct sun | -5 to -10 °C | Avoids surface degradation |
Measure the plate with a contact thermometer, not the controller display. A plate reading 225 °C on screen and 205 °C at the surface produces cold fusion on every joint of the shift, and nothing on the machine will tell the operator.
The Four Time Values And When Each One Starts
| Value | Field rule | What it controls |
|---|---|---|
| Bead-up | Until bead reaches 0.5 + 0.1 x e (mm) | Proves full face contact before timing |
| Heat soak | 10 x e seconds, e in mm | Heat penetration to fusion depth |
| Changeover | 5 s small bore, 8 s above dn250 | Limits melt surface cooling |
| Cooling under pressure | 1 min per mm of wall + 3-4 min | Strength development |
Two mistakes account for most weak joints, and both are timing:
- The timer starts after the bead, not when the plate touches. Pressurise until the collar forms, drop to drag pressure, then count. Timing from first contact adds an uncontrolled 10 to 40 seconds of extra heat.
- Cooling is not optional waiting. Release pressure early and the interface relaxes while still molten. The bead looks fine, the cut face shows voids, and the bend test opens it.
dn160 SDR11, PE100: The Full Set Of Numbers
- Wall thickness e = 14.6 mm
- Bead-up height target = 0.5 + 0.1 x 14.6 ≈ 1.96 mm
- Heat soak = 10 x 14.6 = 146 s
- Changeover ≤ 5 s
- Cooling under pressure = 14.6 + 3 ≈ 17.6 min
- Finished bead height = 0.2 to 0.25 x 14.6 ≈ 2.9 to 3.7 mm
That cooling time is why a crew on dn160 completes 15 to 18 joints in an eight-hour day once facing, alignment and inspection are added. Crews reporting 40 joints on the same diameter are shortening cooling, and the leak appears after backfill rather than before it.
Bead Geometry Is The Only In-Process Evidence
| Check | Target | What a deviation means |
|---|---|---|
| Bead height | 0.20 to 0.25 x e | Low: under-heated or low pressure. High: over-pressure |
| Bead width | Even all round | Uneven: misalignment or unequal plate contact |
| Bead root | Smooth transition, no notch | Sharp notch concentrates stress |
| Bead layers | One homogeneous mass | Layered or stepped: false fusion |
| Cut section | No voids, no unbonded line | Any visible interface line: reject |
Photograph the bead before backfill. On disputed projects bead photographs settle the question faster than any test report, and they cost nothing to keep. Joint acceptance is normally confirmed later by hydrostatic pressure testing.
Adjustments For Wind, Rain, Heat And Cold
| Condition | Adjustment |
|---|---|
| Wind above 15 km/h | Shelter the machine, +5 °C plate, shortest changeover |
| Rain | Stop. Water on plate or end face guarantees a cold joint |
| Below 5 °C ambient | +5 to +10 °C plate, +10 to +20 % heat soak, longer cooling |
| Above 38 °C | -5 to -10 °C plate, +20 % cooling, shade the pipe |
| Pipe stored in sun vs shade | 20 to 30 °C surface difference: let it equalise |
The machine does not know any of this. Parameter discipline is a human task, and it is the reason two crews with identical equipment produce different joint quality on the same main.
The Wall x 10 Rule Is An Approximation
10 seconds per millimetre is a field rule, not a standard value. ASTM F2620 and ISO 21307 publish heat soak tables by wall thickness and pressure regime, and they diverge from the linear rule at both extremes: thin walls are relatively over-heated by the formula, thick walls slightly under-heated. Use the rule for planning and the manufacturer's table for the welding procedure specification.
Our machines ship with the plate thermometer, the three-pressure schedule and the bead chart, so the crew is not converting formulas on the trench edge. See the butt fusion and electrofusion ranges.
Frequently Asked Questions
What is the heat soak time for 160 mm PE pipe?
For dn160 SDR11, e = 14.6 mm, the field rule gives 146 seconds. Confirm against your welding procedure: the accepted range typically falls between 140 and 170 seconds depending on the standard applied.
Can I weld HDPE at 200 °C if the plate heats slowly?
No. Lower plate temperature at the same heat soak time under-heats the interface. Repair or replace the heater, do not compensate with time.
Why does a joint look perfect and fail a bend test?
Changeover time or a contaminated end face. Neither leaves a visible mark on the outside bead, which is why cutting a sample is the only reliable check.
How long before backfill?
Once the joint is below 40 °C, practically the full cooling time plus a handling allowance. Backfilling a warm joint with cold wet soil induces thermal shock.
Butt fusion machines with the three-pressure schedule, calibrated gauges and the bead chart on the panel, from dn63 to dn1200. Tell us the diameter range and the joint volume and we will quote the right class.
Send Inquiry