Electrofusion Welding Procedure: Five Steps That Hold Pressure

Nov 03, 2026

Leave a message

Electrofusion · Method
Electrofusion Welding Procedure: Five Steps That Hold Pressure

Electrofusion joints fail for reasons that are all decided before the welding unit is switched on. The melt cycle is controlled by the machine. The preparation is controlled by the fitter, and it is where the failures come from.

This is the sequence we train crews on: two markings, three fits, five steps. For the alternative, see how the three HDPE jointing methods compare.

0.1 - 0.2 mm
Scrape depth
+10 - 20 mm
Scrape past insertion depth
±0.5 V
Permitted output deviation
Step 1

Mark The Scrape Zone And Remove The Oxide Layer

Mark the area to be scraped on the pipe, then scrape to a depth of 0.1 to 0.2 mm over a length of insertion depth plus 10 to 20 mm.

The extra length matters: the scraper cannot clean exactly at the pipe end, and the fitting body sits slightly proud of the socket. Scraping only to the insertion line leaves a ring of oxidised material at the cold end of the melt zone, which is where a joint starts to peel.

Use a proper scraper. A knife leaves a helical groove that traps air; abrasive paper leaves grit in the interface. Both produce joints that pass a short pressure test and fail a bend test.

Step 2

Mark The Insertion Depth

Measure the socket depth of the fitting and mark it on the pipe. When the pipe is fully inserted, the mark must finish flush with the fitting mouth.

  • Mark short of the socket: the heating coil sits outside the melt zone and the joint is cold at one end.
  • Push past the mark: the pipe bottoms out, displaces the coil and the fitting smokes.

Under-insertion and over-insertion are the two most common causes of a smoking fitting, and both are visible before the machine is connected.

Step 3

Clean, Fit And Clamp

Wipe the scraped surface and the inside of the fitting with clean alcohol and a lint-free cloth, then do not touch either surface. Skin oil is enough to spoil the interface.

Insert to the mark and clamp. The clamp holds concentricity through the cycle: without it the melt can push the pipe off-axis and open a gap on one side. Above dn90, clamping is not optional.

If the pipe has to be forced into the fitting, the cut is not square. Re-cut rather than force it. The fittings themselves, from couplings and tees to saddles and transition pieces, are dimensionally consistent, so misalignment almost always traces back to the pipe end.

Step 4

Connect The Terminals At The Correct Pin Size

Electrofusion terminal pins come in 4.0 mm and 4.7 mm. Fittings up to dn50 usually take 4.0 mm; dn63 and above usually take 4.7 mm. Match them, and push the connector fully home.

Condition What happens
Pin loose in terminal Arcing, localised heat, oxidised contact, erratic resistance reading
Oversize pin forced in Damaged terminal, high contact resistance, output open circuit fault
Pin blackened or pitted Already arced: replace the pin before welding

On plug-type connectors with grub screws, tighten both. Tinning the cable end improves contact on a marginal pin but is not a substitute for the correct size.

Step 5

Enter The Parameters And Stay With The Joint

Enter the fitting data by barcode scan or manually. Check the mode: constant voltage if the label shows volts, constant current if it shows amps. Set the stage count before entering values, then start.

  • Output voltage on the display against the setpoint. Drift beyond 0.5 V means machine or supply.
  • The observation indicator: it should rise steadily and finish fully extruded, typically 5 to 7 mm.
  • The fitting body: warmth is normal, smoke or a hot spot at one terminal is not.

A fully extruded indicator proves the melt reached the indicator cavity. It does not prove the pipe was inserted to depth on both sides, which is why steps 1 to 3 get more training time than the indicator.

After The Cycle

Cooling, Records And Testing

Do not move, twist or water-cool the joint. Leave it clamped and let it reach ambient: 10 to 20 minutes is typical, longer on large fittings and in cold weather. Pressure testing before the fitting is at ambient temperature tests a joint that has not finished forming.

Record the fitting barcode, machine ID, fitter and parameters. On gas work this record is auditable, and it is the document that decides whether a disputed joint is cut out or accepted.

For diameter and SDR context on the pipe side, see SDR11 versus SDR17 versus SDR21.

FAQ

Frequently Asked Questions

How deep should I scrape for electrofusion?

0.1 to 0.2 mm, over the insertion depth plus 10 to 20 mm. Enough to remove the oxidised layer, not enough to change wall thickness.

What happens if I weld without clamping?

The melt can displace the pipe. The joint may look complete and fail at the interface during a bend or pressure test.

Can I weld an electrofusion fitting in the rain?

Only under a shelter. Water at the terminals causes arcing; water in the interface causes steam voids.

Do I need to re-scrape if the pipe touches the ground?

Yes. Contamination is not visible. Re-scrape, re-clean, then insert.

Fittings Made For The Procedure Above

Electrofusion couplings, tees, saddles and transition fittings from dn20 to dn1200, moulded to the SDR and grade your line needs, with the barcode parameters that match the procedure.

Zhejiang Qingfa Pipe Technology Co., Ltd. · www.qingfaindustry.com · +86 151 6813 1515