A leachate system fails at its joints, at the points where the waste mass moves, and where a solvent was buried with the waste. This page works through those three, then gives the families, the size tables and the ordering checklist that answer them.
What actually fails in a leachate line
A leachate system is designed for a thirty-year life, and almost nothing that fails in it fails because the material could not take the chemistry. Leachate is around 99 percent water. The rest is ammonia, chloride, sulphide, dissolved organics and heavy metals at concentrations that matter to a treatment plant and not very much to PE100. The three things that do fail are all duller than corrosion, and all three are decided before the pipe is delivered.
The first is the joint. A collection lateral is laid in a drainage blanket, in wet conditions, in a trench that the machine can barely reach. A joint made badly there is the leak. The second is movement. A landfill settles, unevenly, for twenty years after it closes, and a line that is restrained between a concrete manhole and a liner wall takes that settlement as a bending load at a fixed point. The third is what else was buried. Industrial waste co-disposal puts solvents and hydrocarbons into the same cell, and PE does not corrode in them, it swells and lets them through. That is a permeation problem, not a chemical resistance problem, and no datasheet column covers it.
So this page is organised around joints, movement and permeation rather than around a material comparison. The families are still listed in full further down, but if the pipe is already chosen, the useful part is the position table and the settlement detail.
The range, grouped by where it goes in the cell
The groups below follow the route the liquid takes: from the drainage blanket, into the header, out through the sump, and up to the treatment plant. The gas side is separated out because a gas header is a gas line and is specified as one.
| Family group | Families | Size range | Size entries | What it covers |
|---|---|---|---|---|
| Collection laterals and branches | 8 | dn20–dn1400 | 264 | Couplings, elbows, tees, reducers, flange adaptors and end caps that fuse with a hand tool in a narrow trench. |
| Header and forcemain | 7 | dn20–dn1600 | 324 | The main run out of the drainage blanket and the pumped line to the plant. |
| Branches on a live header | 6 | dn63–dn400 | 68 | Saddles that fuse onto an existing header without cutting it. |
| Gas collection | 3 | dn63–dn400 | 22 | Condensate traps, crosses and vented valves for the gas header and well heads. |
| Isolation | 3 | Ø32–Ø355 | 27 | Fusion-end ball valves at the sump and at each plant inlet. |
| Sump and pump station | 6 | dn25–dn355 | 116 | Steel-to-PE transitions, straight and bent, SDR11 and SDR17. |
| Flanged connections | 5 | dn40–dn1600 | 97 | Stub ends, flange adaptors and steel rings at penetrations and plant skids. |
Position by position, from the blanket to the plant
This is the list we quote against. Each row is a place where the choice is actually made, and the reason is different in each row.
| Position | Fitting that goes there | Why this one |
|---|---|---|
| Collection lateral in the drainage blanket | Electrofusion coupling, tee or 45° elbow, dn110–dn315 | No room for a butt fusion machine between the geotextile and the liner. Electrofusion needs a hand tool and about 150 mm of clearance. |
| Lateral joining a header inside the waste mass | Electrofusion saddle on the header, or a reducing tee if the header is being built at the same time | A saddle goes on after the header is laid and does not cut it. Inside the waste mass, a cut header cannot be re-tested. |
| Header in the drainage blanket | Butt fusion pipe, tees, reducers, dn315–dn630 | Long runs, few joints, and the trench is open for the machine. Lowest cost per joint and the joint has the full pipe wall. |
| Penetration through the liner or a manhole wall | Flange adaptor or stub end with a backing ring, plus a gas-tight boot | The structure is concrete or HDPE, and the penetration is the one place a leak reaches groundwater. Flanged, so it can be dismantled and re-sealed. |
| Sump and pump suction | Butt fusion 90° or 45°, then an equal tee for the second pump | Short, awkward geometry that is built once and never seen again. Fully fused, no mechanical joints below the leachate level. |
| Pump discharge, first 20 m | Steel-to-PE transition, then a 45° rather than a 90° | The pump flange is steel and the forcemain is PE, so the transition is where the two meet. It is also where pulsation and any settlement movement arrive together. |
| Forcemain to the treatment plant | Butt fusion pipe and fittings, dn90–dn315 | Pressure duty, often the highest in the system, and usually SDR 11 rather than SDR 17. |
| Isolation at the sump and at each plant inlet | PE ball valve with fusion ends, Ø32–Ø355 | Fusion ends make the valve part of the line rather than a flanged break in it, which matters where the line may move. |
| Gas well head and gas header | Condensate trap, equal tee, ball valve with vent, dn63–dn400 | Landfill gas carries water vapour that condenses in the header. The trap is a low point, not an accessory. |
| Gas header to the flare or the gas engine | Butt fusion or electrofusion to the plant skid, then a flanged transition | Specified as a gas line, to EN 1555, not to the leachate specification. |
What leachate does to PE100, and what it does not
The useful way to read this table is by exception. Almost everything in leachate is a non-issue for PE100 over the design life; the rows that matter are the ones where the answer changes, and those are the rows worth writing into a specification.
| Constituent | Typical in leachate | PE100 | What it means in practice |
|---|---|---|---|
| Water | balance | No effect | The carrier. Everything below is a minority fraction, which is why leachate is milder than its smell suggests. |
| Ammonia nitrogen | 500–3,000 mg/L | Resistant | No wall loss. Ammonia is a problem for the treatment plant and for odour, not for the pipe. |
| Chloride | 1,000–10,000 mg/L | Resistant | This is the reason the line is PE and not stainless. 316L stress-corrodes above roughly 1,000 mg/L chloride once the temperature passes about 60°C, and leachate sits in that window. |
| Sulphide and hydrogen sulphide | up to several hundred mg/L | Resistant | Attacks concrete and steel, not PE. It is the reason the manholes are lined and the pipe is not. |
| Sulphuric acid from sulphide oxidation | pH 2–4 in the headspace condensate | Resistant at this dilution | Dilute acid is not a problem. The concentrated acid used for cleaning is a different question and should be checked before it is poured in. |
| Methane and carbon dioxide | 50–60% and 35–45% by volume | Resistant, but permeable | PE does not stop methane, it slows it. A gas header is specified as a gas line with a leak test, not assumed tight because it is fused. |
| BTEX, chlorinated solvents from co-disposal | trace to percent | Swelling and permeation | The one row that can rule PE out. Aromatic and chlorinated hydrocarbons permeate PE100 and soften it; where they are expected, the line needs a barrier pipe or a different material. |
| Concentrated oxidising acid, ozone | not present in leachate | Not resistant | Only relevant to cleaning and disinfection procedures. Check the chemical before the first clean, not after. |
Two footnotes that belong with any table of this kind. Resistance here means no significant loss of wall or strength over the design life at the stated temperature; it is not a statement about permeation, which is a separate mechanism and is covered by the methane and solvent rows. And where a cell takes industrial waste, the chemical resistance question is answered by the waste inventory, not by the word leachate. Send the analysis and the answer is specific; guess from the category and it is not.
Temperature: the number that is usually left out
Leachate in an active cell runs warmer than the ambient air because the waste is still decomposing. 30 to 45°C is ordinary, and pockets above 55°C occur where a cell is deep and the cover is thick. PE does not lose chemical resistance at those temperatures, but it does lose pressure rating, and the loss is not small.
| Service temperature | Derating factor | SDR 17 (PN 10 at 20°C) | SDR 11 (PN 16 at 20°C) |
|---|---|---|---|
| 20°C | 1.00 | 10.0 bar | 16.0 bar |
| 30°C | 0.87 | 8.7 bar | 13.9 bar |
| 40°C | 0.74 | 7.4 bar | 11.8 bar |
| 50°C | 0.60 | 6.0 bar | 9.6 bar |
| 60°C | 0.45 | 4.5 bar | 7.2 bar |
The table is indicative and follows the published PE100 water derating curves; for a chemical service the resin supplier's own curve governs, and it should be asked for rather than assumed. The practical consequence is simple. A forcemain designed at 8 bar and installed as SDR 17 has no margin left at 45°C, and the fix is to go to SDR 11 at the design stage rather than to add a thicker wall later. On the gravity side the same logic applies to stiffness rather than pressure, and a warmer, deeper burial is where a deflection problem shows up first.
Settlement is the design load, not pressure
A landfill settles by 10 to 25 percent of its height over the decades after it closes, and it does not settle evenly. Half a metre to two metres of differential movement across a bay is normal, and it arrives at the buried line as a combination of bending and shear that no pressure calculation covers.
PE is the right material for this, but only if the line is detailed to move. A fused PE line bends, and a bend is a strain the pipe can take. A line restrained between a concrete manhole and a liner penetration has nowhere to put that strain, so it concentrates at the two fixed points and at the first rigid connection beyond them. In practice the failures are at the riser and at the pump connection, which are the two places where PE meets something that does not move.
| Measure | What it does | Where it is worth the cost |
|---|---|---|
| Long-radius bend instead of a 90° elbow at the riser | Spreads the strain over a metre of pipe instead of concentrating it in one moulding | Every riser out of the waste mass. The most effective single detail on the page. |
| Slack, laid in a shallow S, rather than a taut straight run | Gives the line somewhere to go when the ground drops under it | Laterals in a deep cell, where the settlement is largest. |
| No rigid anchor between the liner and the waste mass | Lets the line slide rather than pull on the penetration | Any line crossing the liner. The penetration should take pressure, not bending. |
| Steel-to-PE transition set back from the structure | Puts the one rigid joint in the system where it can be inspected and where the pipe has already shed its movement | Pump chambers and plant inlets. |
| Two 45° elbows instead of one 90° where a turn is unavoidable | Halves the strain at the turn and gives a second joint to absorb it | Sump geometry that cannot be changed. |
There is a number worth putting in the specification here, and it is not a pressure. It is the movement each connection has to accommodate, in millimetres, over the design life. Once that is written down, the detail follows from it; without it, the detail is whatever the installer had on the truck.
Zero leak is a testing claim, not a material claim
The phrase used in every landfill tender is that the system must not leak. PE100 cannot leak through its wall, so the only place a leak can start is a joint or a penetration. That makes the quality plan the substance of the promise, and it is worth stating what it consists of before the price is discussed.
| Check | When | What it catches |
|---|---|---|
| Joint parameter record, one line per fusion | During installation | Nothing by itself, but it is the only way to find the joint that was made at the wrong ambient temperature six months later. |
| Bead and cold-fusion inspection on every electrofusion joint | Before backfill | A joint that fused on one side. The bead tells you before the trench is closed. |
| Pressure test of each lateral and each header section | Before backfill | A joint or a fitting that is not tight. Testing after backfill means excavating the waste to find it. |
| Vacuum or oxygen-deficiency test on the gas side | Before commissioning | Gas leaks, which a water pressure test does not find and which matter at a flare or an engine. |
| Penetration seal test, liner side | After the boot is installed | The one leak path that reaches groundwater instead of the sump. |
The record is what makes the thirty-year statement defensible. A fused joint has no gasket to replace, so if it is right at installation it stays right; if it is wrong, the only evidence that it was made at all is the log. This is also why we quote the fusion equipment and the operator training with a large-diameter package rather than leaving it to the contractor.
The families, with the size each one actually reaches
The table below is what we mould, family by family. Most leachate work sits between dn110 and dn630, so almost every family here is quoted well below its maximum; the dn1600 column exists because a header occasionally ties into an existing large-diameter line, not because a collection system needs that size.
| Family | Size range | Sizes | Largest entry | Where it sits in a leachate or gas system |
|---|---|---|---|---|
| Butt Fusion Reducer | dn50–dn630 | 78 | dn630 | Reducing the header where the hydraulic model allows a smaller bore |
| Butt Fusion 90° Elbow | dn20–dn1600 | 31 | dn1600 | Direction changes inside the drainage blanket |
| Butt Fusion 45° Elbow | dn50–dn1600 | 27 | dn1600 | Bends at the riser, where a 90° would concentrate settlement strain |
| Butt Fusion Equal Tee | dn40–dn1600 | 27 | dn1600 | Branch on the header, or the second pump at the sump |
| Butt Fusion Reducing Tee | dn50–dn1600 | 102 | dn1600 | Lateral into a smaller header without a second reducer |
| Butt Fusion End Cap | dn20–dn1600 | 31 | dn1600 | Line end, future cell extension, pressure test closure |
| Butt Fusion Flange Adapter | dn40–dn1600 | 28 | dn1600 | The flanged end at a penetration or a plant skid |
What a leachate package has to state before it can be quoted
The variable part of a leachate package is not the pipe, it is the number of branches and the number of penetrations. Those are the two lines that move the price.
| What to state | Why it moves the price |
|---|---|
| Cell layout: lateral spacing, header route, sump position | Sets the number of tees, saddles and bends, which is most of the fitting count. |
| Design pressure and the service temperature | Together they fix the SDR. A 45°C forcemain at 8 bar is not SDR 17. |
| Gravity or pumped, section by section | Gravity runs are sized on grade and stiffness, pumped runs on pressure. They are different walls in the same package. |
| Waste inventory, if industrial waste is co-disposed | Decides whether PE100 is suitable at all, before anything else is priced. |
| Penetration details and the structure they pass through | Flange adaptor or stub end, and which flange drilling. A ring drilled to the wrong pattern is scrap. |
| Movement allowance at each connection | Decides whether the detail needs a long-radius bend, and whether the transition is set back. |
| Gas side: header route, condensate low points, flare or engine connection | Gas is quoted as a separate package to EN 1555, with traps and vents counted per low point. |
Frequently asked questions
Is HDPE suitable for landfill leachate?
For the great majority of leachate, yes, and it is the standard choice. Leachate is mostly water with ammonia, chloride, sulphide and dissolved organics, and PE100 is resistant to all of them over a thirty-year life. The two conditions that change the answer are a high service temperature, which lowers the pressure rating rather than the chemical resistance, and co-disposed industrial solvents, which permeate PE rather than corrode it.
Which SDR should a leachate line use?
SDR 17 for gravity collection laterals and headers, where the load is soil and settlement rather than pressure, and SDR 11 for a pumped forcemain. The check that decides it is the pressure rating at the service temperature: SDR 17 is PN 10 at 20 degrees and about 7.4 bar at 40 degrees, so a forcemain designed for 8 bar has to go to SDR 11.
Can PE be used for the gas collection header?
Yes, and it usually is, but it should be specified as a gas line to EN 1555 rather than as part of the leachate package. The differences that matter are the leak test, which is a gas test rather than a water pressure test, and the condensate traps at every low point, because landfill gas arrives saturated and cools in the header.
Does HDPE permeate methane or solvents?
Methane, slowly, and solvents, significantly. PE is not a barrier material, so a gas header is made tight by fusion and then tested, not assumed tight because it is one piece. Aromatic and chlorinated hydrocarbons from co-disposed industrial waste both permeate and soften PE100; where they are expected in quantity, a barrier pipe or a different material is the right answer.
How do you connect a lateral to a header inside the waste mass?
With an electrofusion saddle on the header, because the header is already laid and tested and cannot be cut open again at that point. A saddle fuses onto the outside wall and needs only the branch pipe and a hand tool, which is also what fits in the space between the geotextile and the liner.
What temperature does leachate reach?
Typically 30 to 45 degrees Celsius in an active cell, with pockets above 55 degrees where the cell is deep and the cover is thick. It matters because the pressure rating falls with temperature: roughly 26 percent at 40 degrees and 55 percent at 60 degrees against the 20 degree rating.
Do you supply the perforated collection pipe?
No. We mould the fittings: couplings, tees, elbows, saddles, reducers, valves and transitions. The slotted or perforated carrier pipe in the drainage blanket comes from a pipe extruder, and the slot pattern is usually set by the drainage design rather than by the pipe supplier.
- HDPE fittings for mining and mineral processing – the same families specified for abrasive slurry instead of leachate
- HDPE fittings for geothermal ground loops – the other buried loop where a joint cannot be reached again
- HDPE fittings for drainage and stormwater – cap drainage and surface water, which is a separate system from the leachate line
- HDPE fittings for water supply – the potable duty version, and the specification most leachate tenders copy
- HDPE gas fittings – the gas collection header, specified to EN 1555
- Electrofusion fittings – the range used inside the waste mass, and how the fusion works
- Steel-to-PE transitions – the pump connection and the plant inlet
- PE ball valves – isolation at the sump and on each gas well
- Saddle sizes – outlet sizes for a branch on a live header
- ISO, EN and GB compared – which standard a landfill specification usually cites
- Container loading calculator – how many fittings fit a 20 ft or 40 ft container
- Price lists and dimension tables – the 2026 list in Excel and PDF